of the GH TITAN product series: GH TITAN 3F, GH TITAN Attack, GH TITAN Combat, GH TITAN FLAME, GH TITAN REEL, GH TITAN X-TREME
Please note:
For best results, the area to be repaired should be dry, clean and free of grease.
These repair instructions are intended for the proper and professional handling of repairs to fabric flat hoses of the GH TITAN product series of the manufacturer GOLLMER & HUMMEL GmbH and are to be considered in conjunction with the respective manual of the machine manufacturer of the vulcanization press available to them.
The functionality with hose products of other manufacturers has not been tested and can therefore not be confirmed.
Locate and mark the damaged area. Holes or cuts can be repaired up to a size of 4 mm.
Lay the hose flat on a plane surface and fix it in position. Place the hose patch in the center of the previously cleaned damaged area and mark the patch diameter.
Roughen the hose fabric using sandpaper (abrasive cloth with a grain size of 60/80).
Apply a generous amount of the glue to the damaged area (drops with a diameter of approx. 15 mm) and spread it evenly over the marked area.
Apply patch as previously marked.
Place the damaged area with the patch in the vulcanization press (do NOT remove the release film). Preheat the heating element for 10 minutes. Now move the press jaws together, set the preselection counter to 30 minutes.
For the vulcanization process, a temperature of 145°C (293°F) must be reached at the heating elements.
Subsequently, the repaired hose section must be allowed to cool for a further 30 minutes in the pressed state without the addition of heat.
Optimally, allow the patch to cure overnight. Now the hose can be removed. The repair is complete.